Table 4 Resilient modulus values for various combinations.

From: Sustainable subgrade improvement with calcium carbide residue and rice husk ash

Sr. No.

Composition

Soaked CBR (%)

Resilient modulus, MPa

1

BCS::100

1.98

19.80

2

BCS: CCR::95:5

4.52

45.20

3

BCS: CCR::90:10

8.56

69.55

4

BCS: CCR::85:15

8.98

71.71

5

BCS: CCR::80:20

9.02

71.92

6

BCS: CCR::75:25

9.15

72.58

7

BCS: CCR: RHA::85:10:5

9.98

76.73

8

BCS: CCR: RHA::80:10:10

11.26

82.89

9

BCS: CCR: RHA::75:10:15

12.4

88.17

10

BCS: CCR: RHA::70:10:20

12.8

89.98

11

BCS: CCR: RHA::65:10:25

13.1

91.32