Table 7 Specimen Tensile-to-compressive strength ratio.
Specimen number | Splitting tensile strengthfts /MPa | Cubic compressive strengthfcc /MPa | Tensile-to-compressive strength Ratiofts/fcc | Growth rate |
---|---|---|---|---|
WF-0% | 1.65 | 19.8 | 0.0833 | 0.0% |
CF-0.6% | 1.78 | 23.9 | 0.0745 | -10.6% |
PF-0.3% | 1.91 | 24.3 | 0.0786 | -5.6% |
PF-0.6% | 1.98 | 24.9 | 0.0795 | -4.6% |
PF-0.9% | 2.23 | 26.3 | 0.0848 | 1.8% |
SF-0.3% | 1.93 | 30.5 | 0.0633 | -24.0% |
SF-0.6% | 2.42 | 28.2 | 0.0858 | 3.0% |
SF-0.9% | 4.57 | 29.5 | 0.1549 | 86.0% |